成果简介

棉织物不仅是衣物原料,更是可再生的碳前驱体——将其碳化为自支撑锂离子电池负极,兼具废物高值化与免集流体/粘结剂的双重吸引力。然而一个被长期忽视的问题悬而未决:棉织物的纱线规格、织造密度与组织结构究竟是否会影响碳化电极的电化学性能?若答案为”是”,棉基废弃物的回收就不能盲目混用,而需要基于织物架构的分拣——这正是本文试图回答的问题。基于此,本文,东北大学冶金学院能源与环境材料研究中心(E2MC)Ali Reza Kamali 团队在《ACS Sustainable Resource Management》发表英文名”Commercial Cotton Textile-Derived Carbon Cloth for Free-Standing Lithium-Ion Storage”。研究团队选用 4 种市售平纹棉织物(32 与 40 Ne 纱线 × 疏织/密织构型),在完整保留织造框架的前提下碳化为自支撑、无粘结剂电极(CDC),系统考察纱线尺寸、织造密度指数与组织结构对碳结构与电化学行为的影响。
此外,结构分析证实所得为缺陷丰富的乱层堆垛碳,层间距扩展至 3.97–4.13 Å;电化学测试揭示织物构型带来系统性性能差异——疏织碳布表现出更高的电解液可及性、更低的表观界面阻抗与更高的可逆容量,其根源是织物构造、碳结构、电极负载量与离子可及性的综合作用。经实测,CDC-40L 表现最为均衡:100 mA g⁻¹ 下 200 次循环后面积容量 689.3 μAh cm⁻²,200 mA g⁻¹ 下 1000 次循环后保持 343.1 μAh cm⁻²,电荷转移电阻低至 29.26 Ω;动力学分析揭示混合锂存储机制——高扫速下赝电容贡献占比高达 79.9%(8 mV s⁻¹)。本研究将织物构造确立为棉基碳电极的重要设计与报告参数,并为未来基于代表性棉富集纺织废弃物的分拣标准评估提供了框架。
图文导读

Figure 1.(a) Schematic illustration of the preparation process for valorization of cotton fabrics for Li-ion storage applications. (b, c) Photographs of the tube furnace used for the carbonization of carbon fabric, after the carbonization process: (b) the obtained CDC, and (c) end of the tube, showing the formation of bio-oil.

Figure 2.SEM micrographs of (a) CF-32L, (b) CF-32T, (c) CF-40L, and (d) CF-40T, with identical dimensions indicated in each image, (e) CDC-32L, (f) CDC-32T, (g) CDC-40L, (h) CDC-40T, and (i) CDC-40L after 200 cycles at 100 mA g–1 in the delithiated state. (j) An individual carbon fiber at higher magnification. (k) Cross-sectional SEM image of CDC-40L.

Figure 3.Photographs of (a–d) before and after carbonization, and during (e) the bending test, (f) twisting test, and (g) light-through test after carbonization.

Figure 4.(a) Raman spectra and (b) XRD of CDC samples. (c) FTIR spectra of CDC-40L and (d) residue obtained after carbonization.

Figure 5.Gravimetric GCD profiles of (a) CDC-32L, (b) CDC-32T, (c) CDC-40L, and (d) CDC-40T. (e) Gravimetric and (f) areal charge storage cycling performance of electrodes, recorded at 100 mA g–1.

Figure 6.(a–c) SEM images and (d–h) SEM–EDS elemental mapping of CDC-40L after 200 cycles at 100 mA g–1. (e–h) Elemental distributions of C, O, F, and P, respectively. (i) EDS spectrum acquired from the area shown in (d), with the corresponding elemental composition.

Figure 7.Rate performance of CDC electrodes: (a) gravimetric and (b) areal capacity. Long-term cycling of CDC-40L at (c) 200 mA g–1 and (d) 500 mA g–1.

Figure 8.(a) CV profiles of CDC-40L at various scan rates. (b) Log–log plots of peak current versus scan rate used for b-value determination. (c) Relative capacitive-controlled and diffusion-controlled contributions determined using the Dunn method at different scan rates.

Figure9.(a) Cotton production by country in 2025. (88) (b) Global distribution of porphyry copper deposits. Circles denote the four or five largest deposits in terms of tonnage found in countries with the most significant porphyry copper ore resources. (89) (c) Production and reserves of natural graphite in 2023, from the USGS Commodity survey (USGS, 2023). (90)
小结
在本研究中,通过可控热解工艺,将棉基碳布制备成一种无粘合剂的自立式锂离子电池负极材料,同时保留了其固有的编织结构。研究结果表明,棉纺织品不应被视为可互换的碳前驱体:纱线尺寸、织造密度指数和织造结构会显著影响锂离子的可及性、SEI膜的形成、电荷转移电阻以及循环稳定性。疏松编织结构表现出的特性表明其电解质可及性更高、界面电阻更低且可逆容量更大;而紧密编织结构则表现出与更强的界面反应、更高电阻及更低效率相一致的电化学特征。在所测试的电极中,CDC-32L展现出最高的质量容量(246.7 mAh g–1),而CDC-40L则实现了最佳的综合性能:在100 mA g–1下循环200次后,其面容量达到689.3 μAh cm–2,且未出现结构退化,并在200 mA g–1下循环1000次后仍保持约344 μAh cm –2。动力学分析证实了一种涉及扩散控制插层和表面驱动伪电容的混合型锂离子存储机制。与此前报道的生物质衍生和纺织基碳负极相比,CDC-40L在所测试的电极中展现出最理想的整体平衡性。
这些发现确立了织物结构作为报告中的重要考量因素,并为未来研究提供了一个比较框架,该框架将采用独立控制的纺织参数和具有代表性的富含棉纤维的废弃原料——这一因素在以往研究中常被忽视,此前研究中前驱体仅被描述为“棉布”或“废棉布”。研究还表明,专门生产的棉质纺织品应设计为具有合适的结构,而富含棉纤维的废料在资源化利用前应进行分类。更广泛地说,这种方法为碳电极的制备提供了一条循环、可再生且地理分布广泛的途径,有望降低材料消耗强度,并减少对开采石墨、铜集流体和聚合物粘合剂的部分依赖。
文献:https://doi.org/10.1021/acssusresmgt.6c00488